Characteristic:It is one of the typical sperhard Co hss ,with high hardness and hot hardness,high red hardness and good grindability.
Similar steel grade
标准 |
GB |
JIS |
ASTM |
DIN |
Bohler |
ERASTEEL |
钢号 |
W2Mo9Cr4VCo8 |
SKH59 |
M42 |
S2-10-1-8 1.3247 |
S500 |
EM42 |
Chemical Composition:(%)
C |
W |
Mo |
Cr |
V |
Co |
Mn |
Si |
P |
S |
1.05-1.05 |
1.15-1.85 |
9.00-10.00 |
3.50-4.25 |
0.95-1.35 |
7.75-8.75 |
0.15-0.40 |
0.15-0.65 |
≤0.03 |
≤0.02 |
UNEDR ANNEALED CONDITION
Hardness:HB205-255
Delivery status:
As Cold drawn /Hot rolled /forged,in annealed condition.
Size:
Cold drawn bar:¢2.2-14.2mm
Hot rolled bar:¢8.0-80.0mm
Forged bar:¢81.0-250.0mm
Coil:¢6.5-16.0m
Heat Treatment:
Annealing:
Annealing temperature:860-880℃,keep this temperature by 2-4 hours,then cooling to 600℃ in the speed of 20-30℃/h if after cold drawn precess,suggest add stress relieving annealing process Under the temperature of 600-700℃,keep this temperature by 2 houres.
Quenching & Tempering(salt bath)
Quenching:
Pre-heating in two steps:
Heating temperature under :400-500℃ and 850-900℃
Austenitizing temperature :1170-1190℃
Heating coefficient 10-15sec/mm ,quenching under 580-620℃,then cooling to room temperature.
Tempering:
Tempering temperature under :530-560℃,temperature 3 times, each time 1hour ,then cooling to room temperature.
Note:1.Cutting tools in simple shape which requires high hardness,suggest adopt 1190-1200℃ as quenching temperature,530-540℃ as tempering temperture resulted in HRC 67-69.
2 .Cutting Tools in complex shape (such as milling cutter,tap)suggest adopt 1170-1190℃ as quenching temperature.550-560℃ as tempering temperature,resulted in HRC 66.5-67.5.(with Good toughness)
3 .Straightening under 200-450℃ after Quenching.
Copyright:Jiangsu Tiangong Tools Co., Ltd. Address:Houxiang,Danbei Town,Danyang City,Jiangsu Province,China