Characteristic :It is one of the W-Mo Co hss grade with good cutting character. The res hardness, hot hardness and wearing resistance are all better than W6Mo5Cr4V2.
Similar steel grade
标准 |
GB |
JIS |
ASTM |
DIN |
Bohler |
ERASTEEL |
钢号 |
W6Mo5Cr4V2Co5 |
SKH55 |
M35 |
S6-5-2-5 1.3243 |
S705 |
EM35 |
Chemical Composition :(%)
C |
W |
Mo |
Cr |
V |
Co |
Mn |
Si |
P |
S |
0.87-0.95 |
5.90-6.70 |
4.70-5.20 |
3.80-4.50 |
1.70-2.10 |
4.50-5.50 |
0.20-0.40 |
0.25-0.45 |
≤0.03 |
≤0.02 |
UNDER ANNEALED CONDITIN
Hardness :HB205-255
Delivery status :
As Cold drawn/ Hot rolled/ forged,in annealed condition.
Size:
Cold drawn bar :¢2.2-14.2mm
Hot rolled bar :¢8.0-80.0mm
Forged bar :¢81.0-250.0mm
Coil :¢6.5-16.0mm
Heat Treatment :
Annealing:
Annealing temperature :860-880℃,keep this temperature by 2-4 hours, then cooling to 600℃ in the speed of 20-30℃/h if after cold drawn precess,suggest add stress relieving annealing process.
Under the temperature of 600-700℃,keep this temperature by 2 houres.
Quenching:
Pre-heating in two steps:
Heating temperature under:400-500℃ and 850-900℃
Austenitizing temperature:1180-1220℃
Heating coefficient 10-15sec/mm, quenching under 580-620℃, then cooling to room temperature
Tempering:
Tempering temperature under:540-560℃,tempering 3 times, each time 1hour, then cooling to room temperature.