Usage :TGM2 is suitable for produce in high quality cutting tools,such as hob,knife,and milling cutter.TGM2A is suitable for produce in common cutting tools with high toughness,also suitable for cold-forming tools.M2 is suitable for produce common tools.
Characteristic :It is typical steel grade of W-Mo current hss, with high toughness,good thermal plasticity,high hardness,as well as red gardness and hot hardness.
Similar steel grade
标准 |
GB |
JIS |
ASTM |
DIN |
Bohler |
ERASTEEL |
钢号 |
W6Mo5Cr4V2 |
SKH51 |
M2 |
S6-5-2 1.3343 |
S600 |
EM2 |
Composition :(%)
天工钢号
(Steel grade)
|
平均成分wt%(Average percent)
|
||||
C
|
W
|
Mo
|
Cr
|
V
|
|
TGM2
|
0.88
|
6.15
|
4.85
|
4.05
|
1.85
|
TGM2A
|
0.84
|
6.15
|
4.85
|
4.05
|
1.85
|
M2
|
0.85
|
5.7
|
4.7
|
4
|
1.
|
UNDER ANNEALED CONDITION
Hardness :HB205-255
Delivery status :
As Cold drawn/ Hot rolled/ forged,in annealed condition.
Size :
Cold drawn bar :¢2.2-14.2mm
Hot rolled bar :¢8.0-80.0mm
Forged bar :¢81.0-250.0mm
Coil :¢6.5-16.0mm
Heat Treatment :
Annealing:
Annealing temperature:860-880℃,keep this temperature by 2-4 hours,then cooling to 600℃ in the speed of 20-30℃/h
if after cold drawn precess,suggest add stress relieving annealing process
Under the temperature of 600-700℃ ,keep this temperature by 2 houres.
Quenching & Tempering (salt bath)
Quenching:
Pre-heating in two steps:
Heating temperature under:400-500℃ and 850-900℃
Austenitizing temperature:1185-1225℃
Heating coefficient 10-15sec/mm,quenching under 580-620℃,then cooling to room temperature.
Quenching temperature difference in 5-10℃ between TGM2, TGM2A; TGM2A's quenching temperature is higher than TGM2
Tempering:
Tempering temperature under:540-560℃ ,tempering 3 times,each time 1 hour,then cooling to room temperature.