Characteristic:It is current hss developed in our country .Its service performance is equal to that of W18Cr4V(T1) and W6Mo5Cr4V2(M2).
Chemical Composition : (%)
C |
W |
Mo |
Cr |
V |
Mn |
Si |
P |
S |
0.77-0.87 |
8.50-9.50 |
2.70-3.30 |
3.30-4.40 |
1.30-1.70 |
0.20-0.40 |
0.20-0.40 |
≤0.03 |
≤0.02 |
UNDER ANNEALED CONDITION
Hardness:HB205-255
Delivery status :
As Cold drawn/ Hot rolled/ forged,in annealed condition.
Size :
Cold drawn bar:¢2.2-14.2mm
Hot rolled bar:¢8.0-80.0mm
Forged bar:¢81.0-250.0mm
Coil:¢6.5-16.0mm
Heat Treatment :
Annealing:
Annealing temperature:860-880℃,keep this temperature by 2-4 hours,then cooling to 600 in the speed of 20-30℃/h
if after cold drawn precess,suggest add stress relieving annealing process
Under the temperature of 600-700 ℃,keep this temperature by 2 houres.
Quenching & Tempering (salt bath)
Quenching:
Pre-heating in two steps:
Heating temperature under:400-500 and 850-900℃
Austenitizing temperature:1190-1230℃
Heating coefficient 10-15sec/mm,quenching under 580-620℃,then cooling to room temperature.
Tempering:
Tempering temperature under:540-560℃,tempering 3 times,each time 1 hour, then cooling to room temperature.
Copyright:Jiangsu Tiangong Tools Co., Ltd. Address:Houxiang,Danbei Town,Danyang City,Jiangsu Province,China